A kind of method of twining film with regenerated polythene production
Technical field
The present invention relates to a kind of method of twining film with regenerated polythene production.
Background technology
The winding film of enterprise's production at present, the employing linear low density polyethylene resin is a primary raw material, the prestretched of product is generally 150-300%.Twine film if can produce, can guarantee product quality again, just can realize the recycling economy mode of " resource-product-regenerated resources-reconstituted product " with regenerated resources (regenerated polythene).Make it to have significant environmental benefit, social benefit and economic benefit.
Summary of the invention
The present invention is through production technology innovation and the improvement of raw material technical formula, can utilize the regenerated polythene production that contains slipping agent, opening agent to twine film, the tack of product is not damaged, reduce the production cost that twines film to greatest extent, and product have packaging functions such as antistatic, antiultraviolet, ensiling.
A kind of method of twining film of the present invention with regenerated polythene production, it is characterized in that: the coextrusion process of employing is:
Individual layer expressing technique: 25% regenerated polythene (not containing opening agent, slipping agent), the linear low density polyethylene (LLDPE) of 74.4-74.8% (metallocene linear low density polyethylene of available 5%-10% improves intensity), 0.2-0.6% tackifier;
Two layers of coextrusion process: 95% regenerated polythene and functional master batch, 5% linear low density polyethylene (LLDPE) and tackifier (0.2-0.6% is tackifier, the linear low density polyethylene (LLDPE) of 4.8-4.4%);
Three-layer co-extruded technology: (0.2-0.6% is tackifier, the linear low density polyethylene (LLDPE) of 4.8-4.4% for linear low density polyethylene (LLDPE) of (one deck) 5% and tackifier; (two layers) 10% linear low density polyethylene (LLDPE)s (virgin material) and functional master batch; (three layers) 85% regeneration linear low density polyethylene (LLDPE) or regeneration low density polyethylene (LDPE) and metallocene linear low density polyethylene and functional master batch.
In order to improve the ageing resistace of twining film and the intensity of film, except that the regenerated polythene of individual layer expressing technique does not contain opening agent, the slipping agent, the regenerated polythene of two layers of co-extrusion or three-layer co-extruded technology can contain the interpolation composition of opening agent, slipping agent; Functional master batch is antistatic additive, antiaging agent, ultraviolet screener or antistatic master batch, long-lived masterbatch, color masterbatch; The melt index of used resin raw material is 1.5-1.
The sticking evolutionary approach of twining film of other multilayer single face: (membrane structure: skin) 5% tackifier, LLDPE; (membrane structure: the middle level) 20% LLDPE, metallocene linear-low density polyethylene, functional master batch; (membrane structure: internal layer---this layer can be divided into two layers, three layers, with same manufacture of materials) 75% regenerated polythene, polyethylene, metallocene linear-low density polyethylene, functional master batch.
The invention has the beneficial effects as follows, be primary raw material with the regenerated polythene, twines film with LLDPE, metallocene linear-low density polyethylene improved production.Because the regenerated polythene resin property is relatively poor, adopt the LLDPE improved production, can improve the performance of film, the film prestretched reaches 2-3 doubly; Utilize the metallocene linear-low density polyethylene improved production, can allow the prestretched of twining film reach more than 300%, have higher mechanical strength and puncture resistance.Utilize multi-layer co-extruded production technology,, avoided the opening agent in the regenerated polythene material, the defective that slipping agent destroys the tack of twining film, the tack that has guaranteed to twine film through the raw material mix technique improvement.
The specific embodiment
Step:
Connect power supply → heating → batching → reinforced → start
One. the spice technical recipe
Individual layer expressing technique (per 100 kilograms of proportioning ratios): 25 kilograms regenerated polythene (not containing opening agent, slipping agent), 74.4-74.8 the linear low density polyethylene (LLDPE) of kilogram (metallocene linear low density polyethylene of available 5-10 kilogram improves intensity), 0.2-0.6 kilogram tackifier;
Two layers of coextrusion process (per 100 kilograms of proportioning ratios): 90 kilograms regenerated polythene and 5 kilograms of antistatic master batch, 5 kilograms linear low density polyethylene (LLDPE) and tackifier (the 0.2-0.6 kilogram is tackifier, and the 4.8-4.4 kilogram is a linear low density polyethylene (LLDPE));
Or: the regenerated polythene of 92-89 kilogram and 3-6 kilogram color masterbatch or anti-ultraviolet masterbatch, 5 kilograms linear low density polyethylene (LLDPE) and tackifier (the 0.2-0.6 kilogram is tackifier, and the 4.8-4.4 kilogram is a linear low density polyethylene (LLDPE));
Or: the long-lived masterbatch of the regenerated polythene of 77-85 kilogram and 18-10 kilogram, 5 kilograms linear low density polyethylene (LLDPE) and tackifier (the 0.2-0.6 kilogram is tackifier, and the 4.8-4.4 kilogram is a linear low density polyethylene (LLDPE));
Three-layer co-extruded technology (per 100 kilograms of proportioning ratios): linear low density polyethylene (LLDPE) that (one deck) is 5 kilograms and tackifier (the 0.2-0.6 kilogram is tackifier, the linear low density polyethylene (LLDPE) of 4.8-4.4 kilogram); (two layers) 9.5 kilograms of linear low density polyethylene (LLDPE)s (virgin material) and 0.5 kilogram of antistatic master batch; (three layers) 80 kilograms of regeneration linear low density polyethylene (LLDPE) or regeneration low density polyethylene (LDPE) and metallocene linear low density polyethylene and 5 kilograms of antistatic master batch.
Or: (the 0.2-0.6 kilogram is tackifier, the linear low density polyethylene (LLDPE) of 4.8-4.4 kilogram for linear low density polyethylene (LLDPE) that (one deck) is 5 kilograms and tackifier; (two layers) 9.7 kilograms of linear low density polyethylene (LLDPE)s (virgin material) and 0.3 kilogram of color masterbatch or antiultraviolet masterbatch; (three layers) 82 kilograms regeneration linear low density polyethylene (LLDPE) or regeneration low density polyethylene (LDPE) and metallocene linear low density polyethylene and 3 kilograms of color masterbatches or antiultraviolet masterbatch.
Or: (the 0.2-0.6 kilogram is tackifier, the linear low density polyethylene (LLDPE) of 4.8-4.4 kilogram for linear low density polyethylene (LLDPE) that (one deck) is 5 kilograms and tackifier; (two layers) 8 kilograms of linear low density polyethylene (LLDPE)s (virgin material) and 2 kilograms of long-lived masterbatch; (three layers) 70 kilograms of regeneration linear low density polyethylene (LLDPE) or regeneration low density polyethylene (LDPE) and metallocene linear low density polyethylene and 15 kilograms of long-lived masterbatch.
Two, main temperature is controlled (be about 90-120 minute whole heat time heating time):
The temperature of die head: 230~260 degree (front and back), 230~260 degree (about);
Draping connected body: 230~260 degree;
Barrel zone temperature: 230~260 degree 210~230 degree 3 1) 160~180 degree 2)).
Three, extrusion modling (specification): 450mm* (0.015~0.025) mm; 500mm* (0.015~0.025) mm
Four, packing: adopt carton, polybag, packing such as bag weaved.