The content of the invention
In view of the drawbacks described above of prior art, the technical problems to be solved by the invention are to provide a kind of reflective insulation
Elastic aqueous colorful building coating and preparation method, with reflective insulation, high-weatherability imitates stone material and anti-cracking function, to solve
The deficiencies in the prior art.
To achieve the above object, the invention provides a kind of elastic aqueous colorful building coating of reflective insulation, its feature
It is that the coating includes finished product paint, color point, base paint,
Wherein finished product paint is by water 5.0-10.0%, defoamer 0.1-0.2%, multifunctional assistant 0.1-0.2%, ethylene glycol
1.0-1.5%, coalescents 1.2-1.5%, thickener 0.3-0.6%, bactericide 0.3-0.5%, pure-acrylic emulsion 20.0-
25.0%, mixing coloured silk point 70.0-75.0% is made;
Coloured silk point protects glue 25.0-30.0%, colorful base paint 50.0-55.0% by water 20.0-25.0%, reflection every
Thermocolour slurry 1.0-10.0% is made;
Base paint is by water 40.0-50.0%, cellulose 0.4-1.0%, multifunctional assistant 0.1-0.2%, ethylene glycol 1.0-
1.5%, coalescents 5.0-7.0%, wetting agent 0.2-0.3%, dispersant 6.0-8.0%, defoamer 0.2-0.4%, reflection
Heat-insulated titanium dioxide 0.4-0.8%, kaolin 4.0-8.0%, emulsion 26.0-32.0%, protect glue 5.0-8.0%, thickener
2.0-3.0%, bactericide 0.3-0.5% is made.
The elastic aqueous colorful building coating preparation method of a kind of reflective insulation, it is characterised in that comprise the following steps:
1) 6% protection sol solution is prepared
The running water of formula ratio is added in stirred tank, under the speed conditions of 600-800r/min, is then slowly added to
Protection glue powder aluminium-magnesium silicate, stir about 30min is to uniform;
2) white basis paint is made
Base paint makes and is divided into early stage mashing and two stages of later stage paint, specific as follows:
1. early stage mashing
Water is added in stirred tank by formula ratio, under the speed conditions of 600-800r/min, sequentially add cellulose,
Multifunctional assistant, defoamer, wetting agent, dispersant, ethylene glycol, coalescents, titanium dioxide, reflective insulation powder, coarse whiting, lifting turn
Speed to 1200-1500r/min disperse about 30 minutes, near below the 40um of fineness;
2. later stage paint
After above slurry system fineness is qualified, by formula ratio add emulsion, protection sol solution, defoamer, thickener and
Bactericide, regulation system viscosity is suitable;
3) colorful granulation
More than 4 parts of above-mentioned white basis paint is weighed respectively, by stone surface effect, with as reflective insulation mill base phase modulation
Coloured silk point color;
Get off and weigh water by formula ratio, protect sol solution, and above-mentioned color-mixed base paint, under conditions of vacuumizing, mistake
Screen cloth 2-3 times puts size requirements until reaching coloured silk, if color point is not of uniform size, it is necessary to be fabricated separately;
4) multi-color is done
Weigh water, defoamer, ethylene glycol, coalescents, emulsion, above-mentioned colorful particle, sterilization 3) successively by formula ratio
Agent, is well mixed after adding, and finally adjusts viscosity suitable.
The beneficial effects of the invention are as follows:
The suitable building exterior wall surface insulation of the present invention is used, and it not only has the imitation marble effect of multicolor finish, also has
There is reflective insulation performance, External Wall insulation, cracking resistance and imitative stone decoration have important meaning.
The technique effect of design of the invention, concrete structure and generation is described further below with reference to accompanying drawing, with
It is fully understood from the purpose of the present invention, feature and effect.
Specific embodiment
A kind of elastic aqueous colorful building coating of reflective insulation, it is characterised in that the coating include finished product paint, color point,
Base paint,
Wherein finished product paint is by water 5.0-10.0%, defoamer 0.1-0.2%, multifunctional assistant 0.1-0.2%, ethylene glycol
1.0-1.5%, coalescents 1.2-1.5%, thickener 0.3-0.6%, bactericide 0.3-0.5%, pure-acrylic emulsion 20.0-
25.0%, mixing coloured silk point 70.0-75.0% is made;
Coloured silk point protects glue 25.0-30.0%, colorful base paint 50.0-55.0% by water 20.0-25.0%, reflection every
Thermocolour slurry 1.0-10.0% is made;
Base paint is by water 40.0-50.0%, cellulose 0.4-1.0%, multifunctional assistant 0.1-0.2%, ethylene glycol 1.0-
1.5%, coalescents 5.0-7.0%, wetting agent 0.2-0.3%, dispersant 6.0-8.0%, defoamer 0.2-0.4%, reflection
Heat-insulated titanium dioxide 0.4-0.8%, kaolin 4.0-8.0%, emulsion 26.0-32.0%, protect glue 5.0-8.0%, thickener
2.0-3.0%, bactericide 0.3-0.5% is made.
As shown in figure 1, a kind of elastic aqueous colorful building coating preparation method of reflective insulation, it is characterised in that including
Following steps:
1) 6% protection sol solution is prepared
The running water of formula ratio is added in stirred tank, under the speed conditions of 600-800r/min, is then slowly added to
Protection glue powder aluminium-magnesium silicate, stir about 30min is to uniform;
2) white basis paint is made
Base paint makes and is divided into early stage mashing and two stages of later stage paint, specific as follows:
1. early stage mashing
Water is added in stirred tank by formula ratio, under the speed conditions of 600-800r/min, sequentially add cellulose,
Multifunctional assistant, defoamer, wetting agent, dispersant, ethylene glycol, coalescents, titanium dioxide, reflective insulation powder, coarse whiting, lifting turn
Speed to 1200-1500r/min disperse about 30 minutes, near below the 40um of fineness;
2. later stage paint
After above slurry system fineness is qualified, by formula ratio add emulsion, protection sol solution, defoamer, thickener and
Bactericide, regulation system viscosity is suitable;
3) colorful granulation
More than 4 parts of above-mentioned white basis paint is weighed respectively, by stone surface effect, with as reflective insulation mill base phase modulation
Coloured silk point color;
Get off and weigh water by formula ratio, protect sol solution, and above-mentioned color-mixed base paint, under conditions of vacuumizing, mistake
Screen cloth 2-3 times is until reach color point size requirements.If coloured silk point is not of uniform size, it is necessary to be fabricated separately;
4) multi-color is done
Weigh water, defoamer, ethylene glycol, coalescents, emulsion, above-mentioned colorful particle, sterilization 3) successively by formula ratio
Agent, is well mixed after adding, and finally adjusts viscosity suitable.
Include base treatment by the colorful building coating application of the elastic water with reflective insulation effect of the invention, criticize and scrape greasy
Son, applies transparent confinement priming paint, applies reflective insulation floating coating, spray reflective insulation multi-color and the part of roller coating finishing varnish 6, specifically such as
Under:
1) base treatment, the basal plane before construction must be smooth, solid, dries, cleaning;
2) Puttying, Pi Gua 2-3 roads putty are criticized, there is provided a smooth solid basal plane;
3) transparent confinement priming paint is applied, layer of transparent seal coat is applied on the putty for having conserved;
4) painting in reflective insulation is applied, the 2 colorful floating coatings of road reflective insulation is applied on priming paint;
5) reflective insulation multi-color is applied, 2 road reflective insulation multi-colors, room temperature maintenance 2 is sprayed on dry floating coating
My god;
6) finishing varnish is applied, the 1-2 roads resistance to water-white finishing varnish of high durable is applied in the colorful lacquer painting upper roller for having conserved.Specifically
Flow is shown in brief description of the drawings table 1.
Table 1 presses interior wall side's emulsion paint construction process table of this patent production
| Sequentially |
Construction process |
Road number |
It is required that |
| 1 |
Base treatment |
1 |
Smooth, solid, alkalescence is qualified, and humidity is qualified |
| 2 |
Criticize Puttying |
2-3 |
Smooth, solid, alkalescence is qualified, and humidity is qualified |
| 3 |
Roller coat transparent priming |
1 |
Roller coat is uniform, without holiday |
| 4 |
Construction reflective insulation floating coating |
2 |
Construction is uniform, and film is uniform |
| 5 |
Reflective insulation multi-color |
2 |
Coloured silk point is uniform, and form and aspect are consistent |
| 6 |
Finishing varnish |
1 |
Roller coat is uniform, without holiday |
By the colorful building coating of elastic water with reflective insulation effect that the technological process is produced, it is many that performance had both met water
The aeroelastic requirements of color building coating HG/T 4343-2012, reflective insulation performance meets the requirement of GB JG/T235-2014.This
3 kinds of excellent functions above that patent is provided are solved by the following method:
1) reflective insulation function.The reflective insulation effect of the product is to adopt reflection about by reflective insulation multi-color first
The infrared ray of more than 50&, followed by by reflective insulation floating coating reflection about 30% infrared ray, both and together can be by
To in air, performance meets JG/T235-2014 standards to 80% infrared reflection in sunshine, will with reach energy-conserving and environment-protective
Ask.
2) performance of aqueous colorful paint.By from the excellent protection rubber powder of protectiveness, from pliability and excellent weather resistance and hard
The different colorful emulsion of dispersed phase and continuous phase, and the cooperated technique for producing for passing through science, the aqueous colorful paint performance being made meet
HG/T 4343-2012 aeroelastic requirements;
3) anti-cracking function.The anti-cracking function of the patented product is mainly what is realized by following two aspects:During one is elasticity
Apply, performance meets JG/T and reaches GB outer wall building coating JG/T172-2014 II type requirements, and elongation percentage is more than 150%, has
Suitable cracking resistance;Two is the colorful mian paint of water, the emulsion selected by continuous phase and dispersed phase in addition to excellent weatherability,
Also there is certain elasticity, liquid has the ability for covering crackle.Both coordinate together, play the function of effectively covering crackle.
Preferred embodiment of the invention described in detail above.It should be appreciated that one of ordinary skill in the art without
Need creative work just can make many modifications and variations with design of the invention.Therefore, all technologies in the art
Personnel are available by logical analysis, reasoning, or a limited experiment on the basis of existing technology under this invention's idea