[go: up one dir, main page]

CN104073077B - 一种冰点涂料及其制备方法 - Google Patents

一种冰点涂料及其制备方法 Download PDF

Info

Publication number
CN104073077B
CN104073077B CN201410224220.2A CN201410224220A CN104073077B CN 104073077 B CN104073077 B CN 104073077B CN 201410224220 A CN201410224220 A CN 201410224220A CN 104073077 B CN104073077 B CN 104073077B
Authority
CN
China
Prior art keywords
dispersant
calcium carbonate
acrylic emulsion
water
coalescents
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201410224220.2A
Other languages
English (en)
Other versions
CN104073077A (zh
Inventor
高世寒
高致远
高莫凡
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Hebei Chenyang Industry and Trade Group Co Ltd
Original Assignee
ANHUI PROVINCE SEVEN DR CHEMICAL NEW MATERIAL Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by ANHUI PROVINCE SEVEN DR CHEMICAL NEW MATERIAL Co Ltd filed Critical ANHUI PROVINCE SEVEN DR CHEMICAL NEW MATERIAL Co Ltd
Priority to CN201410224220.2A priority Critical patent/CN104073077B/zh
Publication of CN104073077A publication Critical patent/CN104073077A/zh
Application granted granted Critical
Publication of CN104073077B publication Critical patent/CN104073077B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开一种冰点涂料,含有下述重量份的原料:水8-10,醋酸异丁酯18-22,分散剂5027 0.1-0.3,分散剂5040 0.5-0.7,分散剂NNO 0.05-0.15,成膜助剂1-1.4,乙二醇1.8-2.2,增白剂0.05-0.15,有机硅消泡剂0.2-0.4,轻质碳酸钙7-8,钛白粉9-11,高岭土4.5-5.5,重质碳酸钙19-21,滑石粉4.5-5.5,硅丙乳液5.5-6.5,苯丙乳液11.5-12.5,AMP-95 0.05-0.15,聚氨酯增稠剂1-2,防腐剂N-369 0.05-0.15。

Description

一种冰点涂料及其制备方法
技术领域
本发明属建筑装饰材料领域,尤其涉及一种冰点涂料及其制备方法。
背景技术
乳胶漆是水性涂料,以水为溶剂,水在0℃以下就会结冰。通常,乳胶漆的最低施工温度是5℃。低于5℃时,乳胶漆中的主要成膜物质--乳液就无法正常成膜,从而导致涂层出现诸如脱粉、龟裂、卷皮乃至剥落的质量问题。冬季的时候,我国绝大多数地区气温都会远远低于5℃。而此时恰恰时值年底,很多工程工期临近尾声,为了赶工期,很多工人低温施工。于是,就很容易出现内、外墙乳胶漆低温不成膜而造成的施工弊病。结果,不仅工期没赶上,反而给事后的处理带来了很大的困难,颇让施工人员头疼。目前市场上推出的乳胶漆在冬季低温施工时都容易出现的脱粉、龟裂、卷皮、剥落等缺陷。
发明内容
本发明是提供一种旨在解决乳胶漆低温施工易出现的脱粉、龟裂、卷皮及剥落等缺陷的建筑水性冰点内、外墙乳胶漆及其制备方法。
为了实现上述目的本发明采用如下技术方案:
一种冰点涂料,其特征在于,含有下述重量份的原料:
水8-10,醋酸异丁酯18-22,分散剂50270.1-0.3,分散剂50400.5-0.7,分散剂NNO0.05-0.15,成膜助剂1-1.4,乙二醇1.8-2.2,增白剂0.05-0.15,有机硅消泡剂0.2-0.4,轻质碳酸钙7-8,钛白粉9-11,高岭土4.5-5.5,重质碳酸钙19-21,滑石粉4.5-5.5,硅丙乳液5.5-6.5,苯丙乳液11.5-12.5,AmP-950.05-0.15,聚氨酯增稠剂1-2,防腐剂N-3690.05-0.15;
所述的成膜助剂由下述重量份的原料混匀而得:椰壳炭1-2,聚丙烯酸丁酯1-2,天青石粉1-2,蓖麻油0.5-1.3,马来酸二辛酯0.3-0.6,抗氧剂10761-2,抗氧剂1681-2,氢氧化镁0.8-1.2,聚乙烯醇1-2,硅溶胶10-20、环烷酸钴1-1.5、硅酸钠1-2;
所述的成膜助剂的制备方法为:将称取的各原料先于500-700转/分下搅拌混合3-4分钟,于1200-1300转/分下搅拌混合2-4分钟,然后加入适量水,后于300-400转/分下搅拌混合5-8分钟,停止搅拌,即得。
所述的冰点涂料的制备方法,其特征在于:包括以下步骤:
(1)按配方计量在反应釜投入水,开动电机,调整转速在300-500r/min,依次加入分散剂5027、分散剂5040、分散剂NNO、成膜助剂、乙二醇、AMP-95、防腐剂N-369、增白剂、聚氨酯增稠剂,搅拌15-20min;
(2)提高转速到1000-1200r/min。依次加入轻质碳酸钙、重质碳酸钙、高岭土、滑石粉、钛白粉,高速分散30-50min;
(3)经砂磨机研磨到细度≤45um;
(4)在300-500r/min的转速下依次加入硅丙乳液、苯丙乳液、再加入有机硅消泡剂,搅拌20-30min;
(5)加入醋酸异丁酯,过滤,包装,即得。
本发明的原理为:
乳胶漆是水性涂料,以水为溶剂,水在0℃就会结冰。本发明首先选用玻璃化温度不同的两款乳液配伍,并通过特种原材料牵制水分子之间的氢键作用,降低乳胶漆的冰点,使乳胶漆在0℃以下不结冰,再通过调整乳胶漆的挥发速率提高挥发速度,使乳胶漆快速挥发干燥。
本发明的有益效果:本发明从降低乳胶漆冰点和调整乳胶漆挥发速率方面着手,使乳胶漆的最低成膜温度降至-5℃以上,比现有技术条件下的乳胶漆最低成膜温度降低了10℃,可在-5℃以上的条件下成膜,成功地解决了乳胶漆的低温成膜问题,有效的解决了乳胶漆冬季施工易出现的脱粉、龟裂、卷皮、剥落等缺陷,满足了冬季施工的市场要求。
具体实施方式、
一种冰点涂料,含有下述重量kg的原料:
水10,醋酸异丁酯22,分散剂50270.3,分散剂50400.7,分散剂NNO0.15,成膜助剂1.4,乙二醇2.2,增白剂0.15,有机硅消泡剂0.4,轻质碳酸钙8,钛白粉11,高岭土5.5,重质碳酸钙21,滑石粉5.5,硅丙乳液6.5,苯丙乳液12.5,AmP-950.15,聚氨酯增稠剂2,防腐剂N-3690.15;
所述的成膜助剂由下述重量kg的原料混匀而得:椰壳炭2,聚丙烯酸丁酯1,天青石粉2,蓖麻油0.8,马来酸二辛酯0.6,抗氧剂10762,抗氧剂1682,氢氧化镁1.2,聚乙烯醇2,硅溶胶20、环烷酸钴1.5、硅酸钠1;
所述的成膜助剂的制备方法为:将称取的各原料先于700转/分下搅拌混合4分钟,于1300转/分下搅拌混合4分钟,然后加入适量水,后于400转/分下搅拌混合8分钟,停止搅拌,即得。
所述的冰点涂料的制备方法,包括以下步骤:
(1)按配方计量在反应釜投入水,开动电机,调整转速在300r/min,依次加入分散剂5027、分散剂5040、分散剂NNO、成膜助剂、乙二醇、AMP-95、防腐剂N-369、增白剂、聚氨酯增稠剂,搅拌20min;
(2)提高转速到1200r/min。依次加入轻质碳酸钙、重质碳酸钙、高岭土、滑石粉、钛白粉,高速分散50min;
(3)经砂磨机研磨到细度≤45um;
(4)在300r/min的转速下依次加入硅丙乳液、苯丙乳液、再加入有机硅消泡剂,搅拌30min;
(5)加入醋酸异丁酯,过滤,包装,即得。

Claims (2)

1.一种冰点涂料,其特征在于,含有下述重量份的原料:水8-10,醋酸异丁酯18-22,分散剂50270.1-0.3,分散剂50400.5-0.7,分散剂NNO0.05-0.15,成膜助剂1-1.4,乙二醇1.8-2.2,增白剂0.05-0.15,有机硅消泡剂0.2-0.4,轻质碳酸钙7-8,钛白粉9-11,高岭土4.5-5.5,重质碳酸钙19-21,滑石粉4.5-5.5,硅丙乳液5.5-6.5,苯丙乳液11.5-12.5,AMP-950.05-0.15,聚氨酯增稠剂1-2,防腐剂N-3690.05-0.15;
所述的成膜助剂由下述重量份的原料混匀而得:椰壳炭1-2,聚丙烯酸丁酯1-2,天青石粉1-2,蓖麻油0.5-1.3,马来酸二辛酯0.3-0.6,抗氧剂10761-2,抗氧剂1681-2,氢氧化镁0.8-1.2,聚乙烯醇1-2,硅溶胶10-20、环烷酸钴1-1.5、硅酸钠1-2,水适量;
所述的成膜助剂的制备方法为:将称取的各原料先于500-700转/分下搅拌混合3-4分钟,于1200-1300转/分下搅拌混合2-4分钟,然后加入适量水,后于300-400转/分下搅拌混合5-8分钟,停止搅拌,即得。
2.一种如权利要求1所述的冰点涂料的制备方法,其特征在于:包括以下步骤:
(1)按配方计量在反应釜投入水,开动电机,调整转速在300-500r/min,依次加入分散剂5027、分散剂5040、分散剂NNO、成膜助剂、乙二醇、AMP-95、防腐剂N-369、增白剂、聚氨酯增稠剂,搅拌15-20min;
(2)提高转速到1000-1200r/min;依次加入轻质碳酸钙、重质碳酸钙、高岭土、滑石粉、钛白粉,高速分散30-50min;
(3)经砂磨机研磨到细度≤45μm;
(4)在300-500r/min的转速下依次加入硅丙乳液、苯丙乳液、再加入有机硅消泡剂,搅拌20-30min;
(5)加入醋酸异丁酯,过滤,包装,即得。
CN201410224220.2A 2014-05-26 2014-05-26 一种冰点涂料及其制备方法 Active CN104073077B (zh)